Physical Properties
of Tychem® TK
Basis Weight (oz/yd 2)10.6 (ASTM D3776)
Thickness (mils)26 (ASTM D1777)
Ball Burst (lbf)187 (ASTM D3787)
Grab Tensile (lbf)188/180 (ASTM D5034)*
Trap Tear (lbf)53/52 (ASTM D5733)*
* MD/CD

These results are measured by using the latest ASTM test methods. Results will vary due to the changes in test methods.

Tychem® TK
Permeation data for ASTM recommended list of chemicals for evaluating
protective clothing materials (ASTM F1001)
Chemical
Name
Physical
Phase
Normalized
Breakthrough Time
(minutes)
Average
Permeation Rate
(μg/cm2/minute)
AcetoneLiquid>480 <0.01
AcrylonitrileLiquid>480 <0.0003
Ammonia GasGas>480 <0.1
1, 3-ButadieneGas>480 <0.07
Carbon disulfideLiquid>480 <0.02
Chlorine GasGas>480 <0.02
DichloromethaneLiquid>480 <0.03
DimethyllamineGas>480 <0.05
N, N-DimethylacetamideLiquid>480 <0.006
Ethyl AcetateLiquid>480 <0.06
Ethylene Oxide GasGas>480 <0.1
n-HexaneLiquid>480 <0.01
Hydrogen ChlorideGas>480 <0.1
MethanolLiquid>480 <0.1
Methyl chlorideGas>480 <0.02
NitrobenzeneLiquid>480 <0.1
Sodium hydroxide, 50%Liquid>480 <0.1
Sulfuric acid, 98%Liquid>480 <0.1
TetrachloroethyleneLiquid>480 <0.01
TetrohydrofuranLiquid>480 <0.04
TolueneLiquid>480 <0.02

> = greater than, < = less than
For specific permeation data and breakthrough times for other chemicals, contact the DuPont Protective Apparel Fax-OnDemand Service at 1-800-558-9329.

Tychem® TK
Permeation data for 595 Class/Subclass Chemical Warfare Agents
AgentCommon
Name
CAS
Number
ProtocolAverage
Breakthrough
Time
Minimum
Detectable
Permeation
(µg/cm2)
GATabun77-80-6DN5>12hrs.<0.0001
GBSarin107-44-8DN5>12hrs.<0.0001
DN6>12hrs.<0.00024
GDSoman99-64-0DN5>12hrs.<0.0001
DN6>12hrs.<0.0001
HDSulfur Mustard505-60-2DN3>12hrs.<0.0001
DN4>12hrs.<0.2000
LLewisite541-25-3DN3>12hrs.<0.0060
DN4>12hrs.<0.2000
VXVX50782-69-9DN5>12hrs.<0.0001
DN6>12hrs.<0.00024

> = greater than, < = less than

Fabric Test Protocols - All tests performed in triplicate for DuPont Nonwovens by an independant accredited laboratory at 22° C, 50% R.H.
Protocol DN3 - MIL STD-282, Method T-209 (HD) or modified for Lewisite, for 12 hours at 10 g/m 2

Protocol DN4 - MIL STD-282, Method T-209 (HD) or modified for Lewisite, for 12 hours at 100 g/m 2 (Total coverage).

Protocol DN5 - MIL STD-282, Method T-209 (GB) or modified for GA, GD, and VX, for 12 hours at 10 g/m 2

Protocol DN5 - MIL STD-282, Method T-209 (GB) or modified for GA, GD, and VX, for 12 hours at 100 g/m 2 (Total coverage).